Paper No. 670 SELF-COMPACTING CONCRETE -A USEFUL TECHNOLOGY 294 Rizwan, Bier, Ahmad Syed Ali Rizwan, Thomas A Bier, Husnain Ahmad Pakistan Engineering Congress, 70th Annual Session Proceedings 295 296 Rizwan, Bier, Ahmad SELF-COMPACTING CONCRETE -A USEFUL TECHNOLOGY Syed Ali Rizwan1, Thomas A Bier2 and Husnain Ahmad3 ABSTRACT A study on high performance (HP) self-compacting concrete (SCC) is reported. It contains basic information on such systems, their manufacture and applications. The objective of the paper is to introduce this wonderful technology of the decade to the engineers in Pakistan. This technology finds special applications in cases of congested reinforced sections, rafts, highly reinforced columns, bridge piers, tunnel linings, placements and underwater repairs. These are some of the situations where ordinary vibrated concrete can not be effectively utilized. Considering the current pace of research on SCC in the advanced countries it is likely that SCC would replace conventional vibrated concrete in the near future altogether. Unlike most of the published research based on laboratory results only, the information provided in this paper is based on the experience gained in the laboratory, studies made at concrete manufacturing plant and then at the underground placements made in a local tunnel of a teaching and research mine. SCC was pumped therein with a total horizontal (above and below ground level) and vertical distances of 150 meters each. It is interesting to note that a similar SCC formulation gives different response in labo ratory, at plant and then at sites due to differences in mixing regimes, plasticizer activation degree, environmental factors, incorrect estimation of aggregate surface mo isture and its correction at plants, time factor involved in the transportation and onsite waiting and the pumping process of SCC. The results suggest that a thorough understanding of all aspects of this technology is essential for successful SC C production and placements. It is hoped that this single article would provide adequate information on all relevant issues of a durable HP SCC. Keywords High performance concrete, self compacting concrete, superplasticizer, viscosity enhancing agen ts, flow, microstructure, shrinkage and secondary raw materials. 1 Institute for Ceramics, Glass and Construction Materials Technology, Agricolastr, 17, TU Freiberg, 09599, Germany, Professor of Civil Engineering UET, Lahore. E mail: syedalirizwan@hotmail.com 2 Institute for Ceramics, Glass and Construction Materials Technology, Agricolastr, 17, TU Freiberg, 09599, Germany. Professor of Building Materials Technology. 3 Director, NAB, Islamabad. Pakistan Engineering Congress, 70th Annual Session Proceedings 297 INTRODUCTION Despite its wide spread use now in the developed countries, it has been difficult to define high-performance concrete (HPC) in a unified way and no simple and consensus definition exits to date. American Concrete Institute (ACI) defines HPC as the concrete that meets special performance and uniformity requirements that may not always be obtained using conventional ingredients, normal mixing procedures and typical curing practices [1] and these requirements may include enhancement of ease of placement without segregation, long term mechanical properties, early age strength, toughness, volume stability and life in severe environments. Several researchers have de fined HPC in their own way. In this study, like many others, the term HP is used in terms of ease of placement without segregation and is therefore applicable to SCC as well [2,3,4,5]. The vibrated concrete produces differential compaction and hence differential durability. This aspect coupled with shortage of skilled workmen and noisy nature of vibrated concrete were the factors which forced Japanese to think about a concrete that flows by itself without segregation, does not need vibration for full compaction and is environment friendly due to the absence of noise. It was Prof. Okamura and his team from Tokyo university Japan who was able to conceive and produce a powder type of flowing concrete, in early nineties of the previous century. This was called self-compacting concrete (SCC). With the continued research, special flow tests and equipment were designed and specifications were written after detailed testing of this innovative building material which has also been very much liked by the architects due to its excellent surface finish. The main requirements of SCC are very high flow or slump spreads and very high segregation resistance, the two properties which are often contradictory in nature. In the literature, SCC has been classified as po wder type, viscosity agent type and the combination type each differing in the way segregation resistance is achieved. Combination type of SCC uses a moderate powder content and a reasonable quantity of viscosity agent and is considered more robust for structural applications was chosen for local placements in the tunnel. Upto 1940, the maximum concrete streng th at constructions sites was of the order of 20 MPa which had risen to 40 MPa by 1970 and now more than 100 MPA has been used in structures [6,7,8,9,10] .This quantum jump in attainable strength was possible only due to the superplasticizers (SP) which were simultaneously developed in Germany and Japan in late 80’s of the previo us century. The utilization of high performance concrete (HPC) and self-compacting concrete (SCC) has been possible only due to SP availabili ty. In general when such high strengths with sufficient workability are desired, th e maximum size of aggregates should be around 10-12 mm though aggregate size in 12-20 mm range has also been used with water cement ratio in the range of 0.3-0.40[9]. Use of SP, sufficient powder and continuous aggregate gradings are the othe r main ingredients of any HPC or SCC. Continuous grading improves particle pa cking and hence reduces the voids. Lesser 298 Rizwan, Bier, Ahmad voids would require lesser paste and hence lesser water to fill them and to produce a given level of workability. Less paste al so means savings on cement and reduced shrinkage. An improved aggregate packing is indicated when the shape of grading curve starts approximating to a straight line. If the binder phase is also packed, the resulting voids are reduced to a great extent and high performance and self- compacting concretes can be made with improved microstructure resulting in enhanced durability. Unfortunately in mo st of the developing countries SPs are considered to be only the workability enha ncing agents and their main role on the structural durability is seldom recognized by the structural engineers. In addition to SP, secondary raw materials (SRM) or secondary cementitious materials including lime stone powder (LSP ), fly-ash (FA), rice-husk ash (RHA), ground granulated blast furnace slag(GGBFS) or silica fume (SF) are also used.The selection of a typical powder is largely based on required qualities of concrete in both fresh and hardened state. The role of SRMs is to improve packing and hence reduce the water demand of the system. Th ey also replace a part of cement in mortars and concretes resulting in economy, less heat of hydration and hence lower shrinkage. In ready mixed concrete consti tuents, cement is the most expensive, energy intensive and environment unfriendly material. The less energy intensive SRMs being sought are the easily available industrial by-products requiring a little or no pyro-processing and having inherent or latent cementitious properties. Low calcium fly-ash and blast furnace slag have been in the market for a long time whereas high-calcium fly ash, conden sed silica fume, and rice husk ash are relatively new. Use of Fly Ash in concrete is increasing. High cost of cement and pressure from environmental lobbyists are encouraging the use of SRMs to replace cement in concrete. Role of SRMs on SCC performance would be explained in the following text. FILLERS FOR SCC Materials less than 0.125 mm(125 microns) are called powders or fillers and include SF, Fly-ash, ground lime stone(LSP) etc. The fillers should have at least 75% material passing through 0.063 mm sieve for better stability. Various fillers have been employed in the research reported in the literature including lime stone powder (LSP), fly- ash (FA) and ground granulated blast furnace slag (GGBFS). These fillers modify the rheological properties of SCC in fresh state and in the hardened state. When high volumes of lime stone filler are added to SCC mix, the required self-compacting properties are achieved at a lower water/ (cement +filler) ratio. Twenty ei ght days compressive strength is also increased due to filler effect resulting in improved fine-particle packing [11] with LSP particles acting as sites for the nucleation for CH and CSH reaction products. It is reported that the replacement of large volumes of cement by limestone filler (on the order of 100 kg/m 3) is shown to reduce the cement content needed to achieve a given slump flow, viscosity, and compressive strength at early age. The increase in limestone filler content can reduce the HRWRA demand necessary to secure a given deformability. For a given dosage of HRW RA, the loss in slump flow is shown to Pakistan Engineering Congress, 70th Annual Session Proceedings 299 decrease with the increase in lime stone filler in mixtures containing 360 kg/m 3 of cement with the opposite trend observed for concrete with 290 kg/m3 of cement [12]. It has been observed in the laboratory by the authors that calcium carbonate based LSP decreases WD and setting times while dolomite based LSP decreases lesser WD than calcium carbonate based LSP and has no significant effect of setting. The CaCO3 content in LSP was 92.3 % by ma ss. The authors while making a comparative study on the use of different fillers like LSP, FA and FA combinations with SF and RHA found that the use of lime stone filler in self-compacting systems requires the greatest amount of SP for a target flow, gives the least strength, highest linear shrinkage and also has high er maximum pore size [13].This was due to rough and porous nature of LSP , ascertained by SEM and MIP studies, which could retain SP in their bottle necks making it inaccessible to the solution for dispersion purposes. One study suggests that lime stone filler used in SCC does not contribute to strength gain in SCC and is mainly used to increase paste volume without generating excessive heat [14]. It appears that it could be of dolomite based LSP because calcium carbonate based LSP shortens the setting time and would therefore generate more heat than dolomite based LSP or other fillers. It also said therein that SCC columns would have greater ductility but 10% lower strength than similar normal vibrated concrete. It is pr obably due to higher paste content in SCC columns which reduces the modulus in comparison to aggregates it replaces. After a formulation has been arrived at in the light of literature [15], the first step is to carry out the flow tests and these are described now. FA has also been extensively used in making SCC. Low calcium ASTM class F FA generally reduces the water demand, SP content for a target flow, re duces heat of hydration due to delayed setting due to unburnt carbon. SF and RHA can be used with FA by about 20% of its mass to improve flow and strength prop erties. SPs are essential for flow and durability but the information about them is not easily available except the suppliers brochure. Therefore in the follo wing text the necessary information is being provided. MECHANISM OF ACTION OF SUPERPLASTICIZERS There are four main clinker phases of cement namely C 2S, C 3S, C 3A and C4AF and it is reasonable to think that the chemical compounds of these SP’s get grafted on them. In a fresh cement paste without SP, C 2S and C3S have a negative zeta-potential while C 3A and C 4AF have a positive zeta-potential. This leads to a faster coagulation of the cement grains. Cement particles act like a colloid in suspension containing SP. Each colloid carries a “like electrical charge”. Particle charge can be controlled by modifying the suspending liquid characteristics. Modifica tions include changing pH of liquid or changing the ionic species in solution. Another more direct technique is to use surface active agents (SP) which directly adsorb to the surface of colloid and change its characteristics. Calcium aluminate content (C 3A &C 4AF) along with cement fineness effects the fluidi ty in addition to C 3A/ CaSO4 ratio Deflocculation test as described in [16] is able to predict more accurately, the minimum active dosage of 300 Rizwan, Bier, Ahmad an admixture to retain fluidity. A simpler hydrometer tests is also proposed to assess the relative effectiveness of the pl asticizing admixtures[17].The literature also cites that lower alkali content along with lower C 3A+C4AF and higher SO 3 contents give higher fluidity[18]. These ar e the conditions suiting the SP to remain in the solution. Some studies on sulfonat ed polymers of naphthalene, melamine and styrene show that the polymer which is least adsorbed(with highest molecular weight) gives highest negative zeta potential and higher dispersing capacity[19].However, this is not true fo r PCEs’ which have lower zeta potential than SNF and SMF type of super-plasti cizers. The addition method (time of addition) of traditional superplasticizer s is an important factor determining workability of SMF and SNF type superplast icizers. To obtain high workability, their addition should be delayed and op timum time is the beginning of dormant period. However with PCE’s the time of addition is less important to obtain higher workability [20]. The enhanced effect of superplasticizer when added a few minutes after the mixing water, can be explained in a simple way. When SP is added along with the mixing water the SP is rigidl y attached in substantial amounts by C 3A- gypsum mixture leaving only small amounts for the dispersion of silicate phases. By late addition, the SP is adsorbed to a less er extent and there will be enough SP left in the solution to promote dispersion of silicate phases and to lower the viscosity of the system. Double Layer Model A “double layer” model explains the electrical repulsion mechanism and helps understand the definition of Zeta potential. A colloid (negative ion, co-ion) will be surrounded by positive ions(counter ions) in the solution. The attraction from negative ion forces some of the positive ions to stick to its surface around colloid. This layer of counter ions is called “stern-l ayer”. Additional positive ions are still attracted by the negative colloid, but with a small equilibrating force, and are now repelled by the stern layer counter ions and by other counter ions which are trying to approach the colloid.. Figure 1 presents the double-layer model. The double layer is formed to neutralize the charged colloid and in turn causes an electrokinetic potential between the surface of the colloid and any point in the mass of a suspending liquid. This is called surfac e potential and is in milli-volts. The electrical potential at the junction of stern and diffuse layer is called “zeta- potential” and is related to the mobility of the particle. Zeta-potential can be quantified by tracking the colloid particle s through a microscope as they migrate in a voltage field. Pakistan Engineering Congress, 70th Annual Session Proceedings 301 Fig. 1 Double layer Model of SP mechanism of action. This dynamic equilibrium results in the formation of a “di ffuse layer” o f coun ter ions over-lapping t he s tern-layer. D iffuse layer is followed by a layer of io ns which are in eq uilibrium with so lution. In a similar but opposite fashion, there is a lack of negative ions in the neighborhood of the surface because they are repelled by the negative colloid. The concentration of co – ions gradually increases with the distance as repulsive forces of colloid are screened out by the positive ions until equilibrium is again reached. The diffuse layer can be visualized as a charged atmosphere surrounding the collo id. The stern layer and diffuse layers are called double-layer. Van der Waals attraction is the resu lt of addi tive forces between the individual molecules in each colloid. Subtracting attractive curve from the repulsive curve, the net interaction curve is obtained. In order to maximize the repulsion to get dispersion, the colloids should be kept at a minimum prescribed distance, by over coming Van der Waals “ attraction”. This may be done by adding surface active agents like SP. Due to addition of SP, the surface potential of all cement phases becomes negative and they start repelling each ot her. PCEs adsorb more selectively to C 3A and C4AF than to C 2S and C3S. That’s why PCEs need a smaller dosage to achieve the same reduction in water content. In addition long polyether side chains lead to a steric repulsive effect between the ceme nt particles and increase the workability. Longer main and si de chains lead to be tter di spersing and water reduction effe ct while having a small effect on setting times. Po lymeric (Steric) Forces When a polymer layer is presen t at th e surface of pa rticles (either adsorb ed or chemically grafted), a repu lsion force can be created whe n the layers on two neighboring particles overlap. This happens whenever the polymer molecules would rather become more compact as the two layers are squeezed together. Polymeric repulsion occurs only when po lymeric stab ilizer layers overlap. The thickness o f these layers is often of the order of 10 nm . In contrast electrostatic do uble layer s can be much thicker if the ion concentration of the medium is low and polymer repulsion potential is quite steep. 302 Rizwan, Bier, Ahmad SHAPE AND GRADING OF AGGREGATES In general the aggregate shap e requir ements for both normal concrete and SCC are the same stating that no more than 15 % of aggregate s could be elongated. According to DIN EN 933-4 an aggregate is considered elongated if t he ratio of length to the maximum thickness is more than 3.0. Fig. 11 The shape of 8-16 mm size of coarse aggregates used in SCC These elongated aggregates can cause increased internal friction, voids and also pipe blockings at times. Such blockages are also caused by bleeding, high coarse/fine ag gregate ratio, and using pipes with di fferent wear [21]. A high elongated aggregate content also needs a higher paste volume for SCC conveyance because paste is the vehicle for the aggregates. Fig 11 sh ows the shape of 8-16 mm size coarse aggregates used in SCC. According to above mentioned DIN standa rd, it was evaluat ed and was found a border line case with 15% elongated aggregates. CALCULATION OF WATER DEMAND OF SCC SYSTEMS The calculation of a system’s water de mand is often the first required SCC design step [22], therefore a simple procedure should be devised for its evaluation. Complicated procedures using sophisticated equipments [23-24] have been reported in the literature for determi ning the wa ter de mand (WD) of the system. For production of durable SCC mixtures it i s important that the water co ntent of the mixture does not exceed the water demand of the system by a bi g m argin. The importance of maki ng SCCS at a mixing water co ntent close to syste m’s WD has already been mentioned. The total WD o f a SCC system is the sum of individual water demands of the powder and the aggregate components. The WD of the powder can be determined by mixing c ement in the selected mass proportions and test with Vicat needle. For determining the water demand of various size fractions of coarse and fine aggregates simple procedures ou tlined in ASTM C 127 and 128 can b e followed. The results can then be added to get the systems W D as shown in table 5.4. Pakistan Engineering Congress, 70th Annual Session Proceedings 303 Example The following amounts of materials were in a typical SCC formulation. Water demand of 1 m³ of SCC was calculated as given in table 1. Table 1: Calculation of the water demand for 1 m³ SCC-mixture Material Amount in SCC mixture (kg/m³) WD of material (% of mass) WD (kg/m³) Cement : fly ash (1 : 0.387 by mass) (380 +147) 527 27.5 145 Aggregate size 0/2 mm 824 1.73 14.25 Aggregate size 2/8 mm 412 0.933 3.84 Aggregate size 8/16 mm 412 1.06 4.37 Total system’s WD 167.5 Mixing water (w/c=0.45) 171 Difference 3.5 ASSESSMENT OF SCC IN FRESH STATE The architectural Institute of Japan established standard specifications for SCC in 1997 as well as guidelines whic h made use of SCC very common. Three basic criteria are required to achieve self-compaction: high deformability, high passing ability and high resistance to segregation. To secure good deformability, it is important to reduce the friction among solid particles during flow. Aggregate interparticle contact can decrease by reducing the aggregate content and increasing the paste volume to maintain high passing ability among closely spaced obstacles. Adequate cohesiveness can be achieved by incorporating viscosity-enhancing agent (VEA) along with HRWRA to control bleeding, segregation and surface settlement. Another way to enhance the cohesion of SCC is to reduce free water content, increase the volume of fines and cement paste or both. Fine materials and fillers with greater surface area than cement can reduce free water content. The incorporation of VEA in the presence of HRWRA requires greater HRWRA content for a given flow level due to reduction of free-water resulting from the long chain polymer molecules of VMA that absorb and fix part of the mixing water, hence increasing the viscosity of the mixture. The dynamic and static stabilities of SCC are also the main functional requirement for adequate production and use. The dynamic stability prescribes the resistance to segregation during transport and placement while the later refers to the resistance of the fresh concrete to segregation and bleeding once the concrete is cast into place and until onset of hardening. The dynamic stability is assess ed by V-funnel flow time, J-ring, L-box, U-Box and pressure bleed tests. For stat ic stability the determination of surface settlement, aggregate segregation and monito ring the in place changes of electrical conductivity are done. The SCC technology is based on adding or partially replacing cement with fine materials like fly-ash, blast furnace slag and SF without modifying the water content. This process changes th e rheological behavior of concrete. In order to achieve a balance between flowability and stability, the particles<150 µm 304 Rizwan, Bier, Ahmad should be between 520-560 Kg/m 3. High powder content i mproves thecohesiveness. SCC offers environmental, social and economic advantages in addition to offering better performances than normal concrete due to increased cementitious materials content and denser ITZ, (Interfacial transition zone between aggregates and pastes) ,faster construction, noise elimination and placements without skilled labor. HRWRA lowers mostly the yield value but results in a limited drop of viscosity making it possible to have highly flowable concrete without significant reductions in viscosity/cohesiveness. Reduction in water-powder (w/p) ratio results in reduction of deformability of cement paste while an increase in w/p secures high deformability but can reduce cohesiveness of paste and mortar necessitating a balance in w/p ratio to enhance deformability without substantial reduction in cohesiveness. Inter-particle friction increases when the concrete spreads thro ugh restricted spacing due to greater collisions between various solid particles. This increases viscosity thus requiring greater shear stress to maintain a given capacity and deformation speed. It is also essential to reduce the coarse aggregate and sand volumes and instead increase the paste volume to enhance deformability. Continuously graded cementitious materials and fillers can also reduce inter-particle friction. Self-compacting concrete offers a rapid rate of concrete placement, with faster construction times and ease of flow around congested reinforcement. The fluidity and segregation resistance of SCC ensures a high level of homogeneity, minimal concrete voids and uniform concrete strength, providing the potential for a superior level of finish and durability to the structure. SCC is often produced with low water- cement ratio to provide high early strength, earlier demoulding and faster use of elements and structures. The elimination of vibrating equipment improves the environment on and near construction and precast sites where concrete is being placed thus reducing the exposure of workers to noise and vibration. The improved construction practice and performance, combined with the health and safety benefits, make SCC a very attractive solution for both precast concrete and civil engineering construction. The reduction in aggregate content necessitates the use of a higher volume of cement that increases cost and temperature during hydration. Therefore SCC often contains high-volume replacements of fly-ash, blast furnace slag, lime stone filler, or stone dust to enhance fluidity and cohesiveness and also limit temperature due to hydration. The combined use of HRWRA and VEA can insure both high deformability and adequate stability required for high filling capacity, good bond with reinforcement and uniformity of in-situ mechanical properties. Viscosity Agents Commonly used VEA in concrete include cellulose derivatives and polysacchrides of microbial sources-in particular welan gum that improve the capacity of the paste to suspend solid particles. Pakistan Engineering Congress, 70th Annual Session Proceedings 305 Mixes containing VEA exhibit shear thinning behavior whereby the apparent viscosity decreases with the increasing shear rate. Once in place shear rate decreases and the apparent viscosity increases resulting in greater stability. It has been reported that SCC mixtures entrap less air than thoroughly vibrated control concrete having identical volumes of water and cementitious materials. Moreover statistically insignificant differences have been observed between the in situ f c/ values of both types of concrete[25].Viscosity modifying admixture (VMA) not only increases the viscosity but also provides mixture robustness and overcomes effects due to poor aggregate shape and grading[26].At a concrete plant even a limited failure in the aggregate humidity estimation will typically generate 10-20 L excess dose of water per m 3 of concrete causing bleeding and segregation in the absence of viscosity agent[27]. The cracking performa nce and behavior under load suggested that in general cast in place compressive strengths of SCC were closer to standard cube strengths than those of ordinary concrete and at service load level and the crack width was wider with greater depth for ordinary concrete beams than for SCC beams[28 ]. Based on a study encompassing 70 SCC formulations with w/cm ratio in 0.35-0.42, performance based specifications have been formulated for structural applications of SCC [29]. Such SCC’s should have a settlement rate of 0.16%/h at 30 minutes corresponding to a maximum 0.5% maximum settlement. Fillers for SCC are very important and brief information on such powders is given in the next article. FLOW TESTS FOR SCC SCC was originally pioneered in Japan and therefore specified flow tests for SCC were basically designed there and are markedly different from those of normal concrete. These tests are now universally performed tests on SCC. Slump Spread It has been suggested [26,30] that sl ump spread in the range of 500-700 mm is usual for SCC. Flow time (T-50 cm) upto 6 seconds is considered good for SCC. However higher time can also be obtained in case of very cohesive mixes. Flow time generally increases with increase in FA content at the same w/cm [26]. As per authors findings reported elsewhere, flow time was found to be a function of particle shape of powders and it can be further i mproved by using a small quantity of SF (say 20% by FA mass) in FA[26].This would also improve setting, strength and microstructure. For a target flow level pozzolanic powder addition in pastes and mortars increases the water demand and hence SP has to be added and its amount depends upon the particle characteristic s. The strength of HP SCP and SCM is increased with such pozzolanic powders and microstructure is refined and the shrinkage also increases [31-33]. Fig 2 shows SEM of FA particles and fig 3 shows general arrangement of the slump test for SCC. It shows the base of Abrams cone to be in touch with steel plate. However as per German literature the Abrams cone is placed on the narrow end down with the obvious advantage of not requiring an additional person to firmly hold the cone while SCC is being put in. Both the versions of slump tests (with narrow end up or down give almost the same slump value). The process involves filling the cone gently and then lifting it and noting the 306 Rizwan, Bier, Ahmad time when spread reaches the 500 mm Φ mark. If cone is li fted correctly and the platform is level, the spread would be a true circle. The total s pread when the flow stops is also recorded. This test is simple to perform and an experienced practitioner can obtain lots of information about a ty pical SCC mix. The total spread gives an idea about the yield while T 50 cm time can be indicative of viscosity. Moreover visual inspection of any water at the rim of spread ca n be an indication of bleeding while uniform dispe rsion of particles and es pecially the uniform presence of coarse aggregate particles in the entire spread and particularly near the extreme periphery gives an idea about segregation resistance and viscosity of the mix. Fig. 3. Slump Test and T500 measurement arrangement Fig. 2. SEM Pictures of FA particles L- box Test Figs 4 and 5 give the general arrangement of the L-Box test. The vertical part of the box is filled with about 12.7 L of con crete and is left for rest for 1 minute [34] as per Canadian practice but German practi ce does not nece ssarily call for this 1 minute wait. The gate separati ng the vertical and h orizontal compartments is then lifted and the concrete flows out through closely spaced rei nforcing bars at the bottom. The gap and size of the bars depends on the maximum size of the coarse aggregate. The time for the leading edge of concrete to reach the end of 600 mm long horizontal section is noted. The height of concrete remaining in the vertical section (h1) and that at the leading e dge (h2) is evaluated. Various sources se t h2/h1 ratio but values between 0.8-1.0 are generally recommended [34]. This test can detect both blocking and stability of SCC mixes. Pakistan Engineering Congress, 70th Annual Session Proceedings 307 Fig. 4 General arrangement of L-Box Test. Fig 5 Elevation and Sectional View of L-Box test arrangement V-Funne l Time Fig. 6 gi ves the general arrangement of the apparatus. Various dimensions and specially those at the bottom are used but mostly the opening size is 65x75 mm at the bottom. The funnel requires about 10 L concrete and is filled gently. Fig 6 General arrangement of V-Funnel test. Fig 7 General arrangement of U-Box Tests The bottom gate is opened either immediately or after 1 minute (German and Canadian practice respectively) and the time required for the concrete to flow through the opening is measured. The flow is considered to be stopped when light is s een through the opening bottom when looking from the funnel top. This test is used to e valuate the ability of the aggregate particles and mo rtar to flow through a continuously reducing section without segregation and blocking. The funnel time between 6-12 seconds is generally desired for SCC [34]. V-funnel 308 Rizwan, Bier, Ahmad time generally decreases wi th increase in w/cm ratio and also with the i ncrease of fly-ash content for a given w/cm ratio [26]. U-Box Test Fig. 7 give s the gene ral arrangement of the apparatus. This test is used to evaluate the narrow opening passing ability of SCC under a particular head of fresh concrete. One minute after filling the ve rtical compartmen t with concrete, the bottom gate is re moved to allo w concrete to flo w into another rising co mpartment through closely spaced reinforcements. After the flow stops, the height of concrete in rising compartment is measured from the bottom of the apparatus to the top surface. This filling height represents the passing ability and non-blocking behavior of SCC. A maximum of this value is 338 mm [34]. The time required to complete the flow in the rising compartment is also noted and it represents the rate of deformability of the concrete. JSCE recommendations stipulate that a SCC concrete sample sh ould have a minimum filling height of 300 mm while the Europeans guidelines propose to measure the differenc e of he ight in both the compartments. The closer this diffe rence is to zero, the better the flow and passing ability of the concrete, however, t his differe nce should not exceed 30 mm [34].Literature also specifies the ranges of values for differen t tests as applicable to SCC as structural concrete [29]. Fig 8. General arrangement of Blocking ring test. Fig. 9 Details of blocking ring apparatus. Blocking Ring (J-Ring ) Test Figures 8 and 9 give the general arrangement of the apparatus and its details. At the base of the slump cone, a conc entric ring can be used to assess the passing ability of concrete through closel y spaced obstacles. The meas urement is carried out as the mean diameter of the concrete spread when the flow stops. Th e Pakistan Engineering Congress, 70th Annual Session Proceedings 309 gaps between reinforcing obstacle bars depe nd on the maximum size of the coarse aggregate. The J-Ring can be used in conjunction with the slump flow to evaluate the passing ability and the amount of spread loss when concrete is made to flow through obstacle rei nforcing bars simul ating the actual placing conditions. The difference between the slump spread and J-Ring spread should not be more than 50 mm (German guidelines) or 10 mm by Euro pean guideli nes [34]. It has been experienced that wh en the shape of coa rse aggregate is rather elongated, it is extremely diffi cult to satisfy the re quirements laid do wn in th e European Guidelines; however, German requirements for this test look reasonable as these seem to take care of the variation in shape of coarse aggregate as well. Fig 10 Air Content Meter The SCC sample is gently put into the container (bottom h alf of the air content meter) approximately upto top by leaving a gap of around 1-2 m m between top of t he concrete a nd the top of bottom half. There should be no aggregate particle or paste at the rim ju nction of top and bottom of the apparatus to provide an air-tight connection between the two ha lves of th e apparatus. After fillin g, the apparatus is rotated an d wobbled without impact so as to release any air. Then water is sprayed into as shown. After that red stoppers are put down and air is pumped by using brown top lever. Correction is done by using top black button (right) and tabbing the glass plate till the needle reads zero. Then green measurement button (left) is pushed and air content is displayed. Ai r Content Fig 10 shows the air content meter used in the investigation. The air content in concrete is an important criterion. Sometimes a higher air content in SCC may be desired to increase the freeze-thaw resistance, however, an air content of around 2- 3% remains entrapped in normal SCC mix depending upon the dosage of SP and VEA and type of powders being used. . Due to various admixtures used, its amount can vary and has to be checked against the design value. In case of discrepancy the mix may be revised. Generally an air cont ent of around 2% in non-air entrained SCC can be consider ed OK. Air content is also important w.r .t pumping procedure. With higher air content induced due to a dmixtures or other ingredients, the yield stress can increase with a correspond ing accompanying plastic viscosity can decrease [35]. EXPERIMENTAL 310 Rizwan, Bier, Ahmad Materi als Many cement types were used by th e authors including CEM I(C I) and CEM II/A-LL 3 2.5R (C II) and har d coal fly-ashes (SRM) were used in v arious SCC formulations. Table 2 gives the properties of powders used. Table 2: Properties of Powders used Powder Particle Size (µm) BET Area (m2/g) Density (g/cc) SiO2 Fe2O3 MgO CaO Al2O3 Na2O K2O LOI % SO3 CI 32.5R 23.7 0.858 3.135 20.29 2.26 1.71 62.45 5.41 0.83 0.72 1.87 3.25 CI 42.5R 18.9 0.81 3.168 18.92 2.27 1.72 63.16 5.09 1.48 1.35 2.34 3.48 CII 16.90 1.353 3.11 18.74 2.23 1.38 58.9 4.78 1.25 1.01 7.09 3.20 FA1 26.59 1.65 2.31 51.44 5.55 2.51 4.03 26.13 1.23 2.63 2.71 - The Bogue’s potential parameters of CEM II/A-LL 3 2.5R are C 2 S= 19.56, C 3 S= 51.18, C3 A= 10.5 and C4 AF= 6.87. These parameters for the other two cemen ts can be easily calculated. Siliceous sand (0-2 mm) and natural gr avel (2-8 mm and 8-16 mm) wa s used for the SCC-mixes. Figure 12 shows the grading curves of sand and of total aggregates. Figure 12 (a): Grading curves of sand (0-2 mm)- Figure 12 (b) Grading of total aggregate used for SCC. Contents of fractions (0-2 : 2- 8 : 8-16 mm):G1 (39:33:28), G2 (45:27:28), G4 (50:25:25),G6 (5:22.5:22.5), The grading curves of aggregates used in this research work with a maximum aggregate size of 16 mm falls within the limits of German standards DIN EN 206-1 and DIN 1045-2 [25] . A random sample of 8/16 mm fraction of aggregates when tested for % elongated material accordin g to DIN EN 933-4 showed about 15 % o f such material. MIXING PROCEDURE Pakistan Engineering Congress, 70th Annual Session Proceedings 311 The mixing sequence consisted of: • Mixing of dry constituents for 30 seconds • Then adding water, superplasticizers and viscosity agent at the same time. • Mixing the ingredients for another 90 seconds. In the laboratory, mix was kept undisturbed for 7 minutes and then 1 minute of final vibration was given for SP ac tivation. F or each tests in fresh state after slump spread, the mix was again given 5 se conds mixing. At plant after 2 minutes, the concrete was poured in the truck and was continuously agitated slowly. After 9 minutes it was given 1 minute of fast truck mixing before starting flow tests at pl ants. At site same sequence was observed before pumping SCC in the tunnel. This may not be the most effi cient mixing regime but it had to be adjusted to the stringent plant mixing pr ocedures wh ich normally do not allow the use of optimal mixing procedures as recommended elsewhere [22]. SCC FLOW TESTING In the fresh state the tests including slump spread (cone standing on narrow end), V-funnel time, L-box and J-ring (block ing ring) were carried out in sequence. After that air conte nt was tested. The a verage time spent on completing the flow tests was around 20 minutes for a three men party. The sample was mixed again for 5 seconds before starting another test after slump test. Figure 13 shows the relation between the admixtures ratio (plasticizer: stabilizer; P/S) and V-funnel time of SCC formulations with CEM II (Fo r powder and aggregate content see table 5.4 and for grading d etails see Fig. 5.10(b).The target slump spreads for G4 and G2 formulations were 66±1 and 70±1 cm respectively. Figure 13: V-funnel time and P/S relation for two aggregate gradings with CEM II 312 Rizwan, Bier, Ahmad The mixing regime in the laboratory was the same as that used at plant. It may not be very efficient though especially the activation of the activation of superplasticizers may not be achieved in a total two minutes of mixing time because of low shear rates of the laboratory mixer and smaller SCC sample volume (50 litres). It is therefore suggested that slump should be taken after the activation of the superplasticizers otherwise the slump te st values (T50 cm and spread) will be incorrect and its comparison with J-ring ma y not be accurate. This can be done to leave the mixed material in the pan upto seven more minutes and then mixing for 1 minute more. Alternatively the total mixing time can be increased fro addressing the issue. Although a final consistence adjustment with water is allowed [22], however laboratory observation showed that even a very small water addition after the addition of admixtures can reduce the mix cohesion and/or could be misinterpreted and may therefore be avoided. Table 3 and 4 show quantities of SCC mixes designed for the stated spreads. Table 3: SCC mix ingredients Mix. No constituents 1 2 3 4 5 6 7 8 9 10 11 Cement-kg/m3 C132.5R,380 C132.5R-380 CII-380 CII-380 CII-380 CII-380 CII-380 CII-380 CI-330 CI-330 CII-380 Water-kg/m3 168 171 171 171 171 171 171 171 148.5 148.5 171 FA kg/m3 147 147 147 147 147 147 147 147 197 197 147 Sand 0-2 mm kg/m3 635 635 635 732 732 732 813 898 919 919 893 Aggregate-2/8 mm kg/m3 538 538 538 439 439 439 406 366 376 376 366 Aggregate- 8/16mm kg/m3 456 456 455 455 455 455 406 366 376 376 366 SP (% cement mass), kg/m3 1.3,4.94 1.8,6.84 1.8,6.8 1.8,6.84 1.9,7.22 1.9,7.22 2,7.6 2.6,9.88 3.4,11.22 4.2,13.86 2.8,10.9 VEA (% cement mass), kg/m3 0.64,2.4 0.89,3.4 0.95,3.6 0.95,3.6 1.05,4 1,3.8 1.3,4.94 1.2,4.56 1.3,4.28 1.3,4.28 1.4,5.32 Grading G1 G1 G1 G2 G2 G2 G4 G6 G6 G6 G6 W/c 0.45 0.45 0.45 0.45 0.45 0.45 0.45 0.45 0.45 0.45 0.45 w/cm 0.32 0.32 0.32 0.32 0.32 0.32 0.32 0.32 0.28 0.28 0.32 Table 4: SCC mix ingredients (contd) Mix.No constituents 12 13 14 15 16 17 18 19 20 21 22 Cement-kg/m3 C1-330 C1-330 CII-340 C1-300 C1-330 C1-300 C11/BM,340 C11/BM, 350 C1-300 C1-300 C11- 340 Water-kg/m3 165 188 153 171 185 171 153 157 171 171 160 FA kg/m3 197 197 187 227 197 227 187 177-2 227 227 187 Sand 0-2 mm kg/m3 896 793 830 887 789 795 829 819 795 795 815 Aggregate-2/8 mm kg/m3 366 397 415 362 394 398 414 414 397 398 408 Aggregate- 8/16mm kg/m3 366 397 415 362 394 398 414 414 397 398 408 SP (% cement mass), kg/m3 3.1,10.3 2.65,8.76 1.91,6.46 2.5,7.5 2.5,8.3 2.4,7.2 2.4,8.15 2.4,8.4 2.3,7.2 2.45,7.35 2.2,7.47 VEA (% cement mass), kg/m3 1.3,4.3 1.35,4.5 1.5,5.1 1,3 1,3.3 1.2,3.6 0.9,3 0.9,3.15 1.25,3.76 1.12,3.36 1.1,3.75 Grading G6 G4 G4 G6 G4 G4 G4 G4 G4 G4 G4 w/c 0.5 0.57 0.45 0.57 0.57 0.57 0.45 0.45 0.57 0.57 0.47 w/cm 0.31 0.35 0.29 0.32 0.35 0.32 0.29 0.29 0.32 0.32 0.3 Pakistan Engineering Congress, 70th Annual Session Proceedings 313 FLOW RESPONSE The flow response of each SCC mix was noted by slump spread, V-funnel time, L-box, J-ring test and air content test in the sequence. All these tests required 20 minutes for a three men party. The SCC mixes were designed for two slump spread ranges, 65-68 cm and 69-72 cm. Table 5 gives flow response of 65-68 cm slump spread mixes while Table 6 gives the flow response of 69-72 cm slump spread. Table: 5 Flow properties of mixes designed for slump spread of 65-68 cm Grading G4 G6 G4 G6 G4 Mix number 7 8 11 12 13 15 19 T50,s Spread,cm 8.5 65 7 68 6 67 9.3 68 6.4 67 8.1 68 8.5 68 Funnel, Time, s 12.8 10.3 15.8 14.6 9.2 12.2 15 L-box T60,s-h2/h1 11 0.93 8.37 0.98 13.4 0.92 14 0.96 7.18 0.98 12.3 0.96 15.9 0.97 J-ring T50, spread. cm 14.8 60 12.3 63 13.3 66.5 20 62.5 8.91 66 16.7 63.4 13.4 66 Air % 2.7 2.9 2.6 2.8 1.9 2.5 2.2 Table 6: Flow properties of mixes designed for slump spread of 69-72 cm Mix 1 2 3 4 5 6 14 17 18 20 21 22 T50,s Spread, cm 6 71 5.5 71 5.6 69 7 70 8 69 7 71 11.5 69 5.8 72 9.2 71 6.7 70.5 6.3 71 9.3 70 Funnel, Time, s 18 12.4 11.6 9 10.7 10.6 18.8 11.8 18.5 10.1 10.3 15.4 L-box T60,s- h2/h1 9 1 9.6 1 6.2 0.96 7 1 7 1 9.2 1 17.5 0.92 12.6 0.96 19.6 0.9 11.4 0.96 9.7 0.93 14.1 0.93 J-ring T50, spread, cm 12 63 7.7 71 8.7 68 10 69 11.5 66.5 11.8 68.5 19.6 63 13.6 63.5 17.9 67.5 11 68.5 12 67 18.1 66.5 Air % 1.0 1.8 1.5 1.7 2.1 1.9 2.5 1.6 2.1 2.1 1.9 2.5 314 Rizwan, Bier, Ahmad Fig. 14 shows the sl ump spread and J- ring spread of SCC mixes pertaining to G4 g rading. I t c an b e s een t hat relationship is fairly good excep t that J- ring values are less than corresponding slump spreads due to obvious blocking effect of the ring. Figure 14: Slump and J-ring slump spreads relation for G4 grading. STRENGTH RESPONSE After casting, the specimens were placed in plastic containers at 20°C and 90%+ relative humidity. Those were de moulded after 24 hours and then put in water till the age of t esting. According to German specificatio ns, concrete has to be taken out of water after 7 days and then air cured at 67% relative humidity at 20°C. How ever as the effect of curing in va rious relative humidity ranges was also studied, 28 days strength of w ater cured samples can be reduced by about 14% to get the strength according to German st andards. Table 7 sho ws the 28 days SCC compressive strength of 10 cm cubes. The differences and the reason s in the flow and strength response of SCC mixes cast in the laboratory, at plant and then at placement site in tunnel by pumping are given elsewhere [15]. Table 7: 28 day compressive strength of some SCC mixes. Mix Number Compressive Strength, MPa 9 80 10 75 11 68 12 70 13 66 15 65 16 68 17 70 18 74 20 68 21 68 22 63 Pakistan Engineering Congress, 70th Annual Session Proceedings 315 Figure 15 gives the relationship of w/c ra tio and co mpressive strength o f G6 mixes wh ile figure 16 explains the e ffect o f relative humidity (at constant temperature of 20°C) on the compressive strength of a typical SCC mix. Fig. 15 28 days w/c-strength relation for G6 grading. Fig 16 Effect of relative humidity(at 20°C) on the compressive strength of SCC. MICROSTRUCTURE Various methods of microstru ctural investigations can be used depending on what is being looked after. Environmental scanning electron microscopy (ESEM) is being increasing used in the studies of microstructure along with x-ray d iffraction (XRD) an d thermal analysis (Thermogra vimetry –TG and differentia l scanning calorimetry- DSC). In a reinforced concrete struct ure the forces are transferred to steel from concrete through bond. Between the paste and aggregate of concrete there exists an area called interfacial transition zone (ITZ) of about 30-50 microns whose properties are different from th e surrounding mortar. Moreov er in this ITZ some water may collect encouraging t he growth of weak Ca(OH) 2 crystals(CH) . Therefore in this entire assemblage, ITZ becomes the weakes t link. Material engineers are trying t o improve the quality of this ITZ by incor porating such SRM (SF, RHA, FA) which react with CH and hence improve the microstru cture. A typical microstructure is shown below. Fig 17: A microstru cture of a t ypical HP SCM system using LSP with CEM I at the age of 28 days is shown . Hydration products (thin needles) and calcium hydroxide crystals (flaky and plate like) are clearly seen. The microstructure growth generally takes place in the pores for a continuously graded and packed formulation. 316 Rizwan, Bier, Ahmad SECONDARY RAW MATERIALS (SRM) FOR SCC IN PAKISTAN A physical survey was carried out to know the availability of SRMs for making SCC in Pakistan. Fly-ash is avail able in a small quantity from the thermal power plants in private sector but it ma y not be economically exploited. The lime stone flour, obtained during crushing of Margallah rocks for making coarse aggregates, is available and can be used ve ry effectively. For the time being it is adding to environmental problems. Ground granulated blast furnace slag can also be an option. Rice husk ash can be made locally and can be used along with LSP for the improvement of resulting SCC concrete. The authors are busy in making tests on locally available SRMs and results will be published in near future. CONCLUSIONS 1. A simple procedure of calculation of water demand of SCC mixes has been developed and used .All HP/SCC mixes must be at a mixing water content equaling that corresponding to the de mand of the system for economy and durability. 2. The shape of coarse aggregate is very important for the flow response of SCC. Elongated coarse aggregates create larger voids in the mix and therefore require higher paste contents for meetin g flow targets. Such aggregates can produce pipe- blocking during pumping if mix is inadequately designed. 3. Mixing regime is very important for making HPC/SCC. The time and sequence of addition of chemical admixtures were also very important. 4. Use of FA reduces cement and hence early shrinkage which is a very big consideration in HPC/SCC. Its spherica l particle shape is useful for flow through congested sections. 5. In the laboratory, the flow measur ements should be ta ken only after the activation of superplasticizer. 6. Increasing SP/VEA ratio increases flow . The flow starts at a typical SP/VEA ratio for a given SCC formulation and further increases do not improve the flow very significantly. 7. SCC mixes were designed for 60 MPA and all mixes had higher strengths by a reasonable margin. 8. The reasons for the response differences of a similar formulation when tested in laboratory, at plant and then at site are attributed to batch size differences, inadequate estimation of aggregate surface moisture, transportation time and waiting at site. Pumping also changes flow response. 9. This technology can be effectively used by the engineers in Pakistan. ACKNOWLEDGEMENTS The authors wish to thank Prof.Dr.Ing. Frank Dahlhaus for providing an opportunity for on site SCC placements in a local tunnel of teaching and research mine. Pakistan Engineering Congress, 70th Annual Session Proceedings 317 REFERENCES [1]. ACI 363R-92, Re-approved 1997. “Sta te-of-the-Art Report on High-Strength Concrete”, ACI, Detroit, USA. [2]. Khayat, K. H., “Workability, Testin g, and Performance of self-Consolidating Concrete”, ACI Material Journal, Vol. 96, No. 3, may-June 1999, pp 346-353. [3]. Su, N.; Hsu, K-C.: and Chai, H-W., “A simple mix design method for self- compacting concrete,” Cement and Concrete Research 31 (2001) 1799-1807. [4]. Khayat, K. H: and Aitcin, P.C., “Use of Self-Consolidating Concrete in Canada”, Proc. International Workshop on Self-Compacting Concrete”, 23-26 August 1998, Japan, pp 11-22. [5]. Bui, V. K., Akkaya, Y., and Shah, S. P., “Rheological Models for Self- Consolidating Concrete,” ACI material s Journal, V.99, No. 6, November- December 2002, pp 549-559. [6]. Atahan, H.N., Oktar, O.N., and Tasdemir, M.A., “The effect of the pore structure of hardened cement paste on the properties of HSCs”, Proceedings of 6 th International symposium on the utilization of high strength/high performance concrete”, Vol. 2, Leipzig, June 2002, pp 839-852. [7]. Bornemann, R., and Schmidt, M., “The role of powders in concrete”, Proceedings of 6 th International symposium on the utilization of high strength/high performance concrete”, Vol. 2, Leipzig, June 2002, pp 863-872. [8]. de Almeida, I.R., “On the influence of the modulus of elasticity of coarse aggregate on the modulus of elastici ty of high performance concrete”, Proceedings of 6 th International symposium on the utilization of high strength/high performance concrete”, Vol 2, Leipzig, June 2002, pp 887-896 [9]. Naik, T.R., and Kraus, R.N., “Te mperature effects on high-performance concrete”, Proceedings of 6 th International symposium on the utilization of high strength/high performance concrete”, Vol. 2, Leipzig, June 2002, pp 1203-1222. [10]. Persson, B., and Terrasi, G.P., “H igh performance self-compacting concrete, HP SCC”, Proceedings of 6 th International symposium on the utilization of high strength/high performance concrete”, Vol. 2, Leipzig, June 2002, pp 1273-1290. [11]. Bosiljkov, V.B., “SCC mixes with poor ly graded aggregate and high volume of limestone filler”, cement and concrete research 33 (2003) 1279-1286 [12]. Ghezal, A. and Khayat, K. H.: Optimizing Self-Consolidating Concrete with Lime Stone Filler by Using Statistical Factorial Design Methods. ACI Materials Journal, Vol. 99, No. 3, May-June 2002, pp. 264-272. [13]. Rizwan, S. A., and Bier, T. A., “H igh Performance Self-Compacting Mortars Containing Pozzolanic Powders”, BMC-8, The Eight International 318 Rizwan, Bier, Ahmad Symposium on Brittle Matrix Composites, 23-25 October 2006, Warsa, Poland. [14]. Khayat, K. H., Paultre, P., and Tr emblay, S., “Structural Performance and In-Place Properties of Self-Consolidating Concrete used for Casting Highly Reinforced Columns,” ACI Materials Journal, V.98, No.5, September-October 2001, pp 371-378. [15]. Rizwan, S. A; Bier, T.A: and Dombrowski, K., “A discussion on the essential issues pertaining to successful development of self-compacting concrete-SCC”, BMC-8, The Eight International Symposium on Brittle Matrix Composites, 23-25 October 2006, Warsa, Poland. [16]. Macias, A: and Goni, S., “Character ization of Admixture as Plasticizer or Superplasticizer by Deflocculation Tes t”, ACI Material Journal, V. 96. No. 1. January-February 1999, pp 40-46. [17]. Magee, B. J: and Alexander, M .G., “Simple test method to assess the relative effectiveness of plasticizing chemical admixtures”, Cement and Concrete Research 31 (2001) 303-307. [18]. Chandra, S: and Bjornstrom, J., “Influence of cement and superplasticizers type and dosage on the fluidity of cement mortars-Part 1,” Cement and Concrete Research, 32 (2002) 1605-1611. [19]. Andersen, P. J: and Roy, D. M., “The Effects of adsorption of superplasticizers on the surface of cement,” Cement and Concrete Research , 17 (1987) 805- 813. [20]. Goaszewski, J: and Szwabowski, J., “Influence of superplasticizers on rheological behavior of fresh cement mortars,” Cement and Concrete Research 34 (2004) 235-248. [21]. Kaplan, D; de Larrad, F. and Sedran , T.: Avoidance of blockages in concrete pumping process. ACI Materials Journal, Vol. 102, No.3, May-June 2005, pp. 183-191 [22]. The European Guidelines for self-compacting concrete, May 2005, 63 pp. [23]. Marquardt, I.; Vala, J. and Diederic hs, U.: Optimization of self-compacting concrete mixes. Proceedings of second International symposium on self- compacting concrete, Tokyo, 2001, pp. 295-302 [24]. Marquardt et al.: Proceedings of first North American Conference on the design and use of self-consolidating concrete. ACBM, USA, November 12-13, 2002. [25]. Khayat, K. H; Manai, K; and Trudel, A., “In-Situ Mechanical Properties of Wall Elements Cast Using Self-Consolidating Concrete”, ACI Materials Journal, V. 94, No. 6, November-December 1997, pp 491-500. [26]. Lachemi, M; Hossain, M.A. H; Lamb ros, V: and Bouzoubaa, N., “Development of Cost-Effective Self-Consolidating Concrete Incorporating Fly Ash, Slag Pakistan Engineering Congress, 70th Annual Session Proceedings 319 Cement, or Viscosity Modifying Admixt ures”, ACI materials Journal, V.100, No.5, September-October 2003,pp 419-425. [27]. Sari, M; Prat, E: and Labastire, J.F., “High Strength self-compacting concrete-Original solutions associatin g organic and inorganic admixtures,“ Cement and concrete research 29 (1999) 813-818. [28]. Sonebi, M; Tamimi, A. K: and Ba rtos, J. M., “Performance and cracking behavior of reinforced beams cast with self-consolidating concrete,” ACI Material Journal, V.100, No.6, November-December 2003, pp 492-500. [29]. Hwang, S-D; Khayat, K.H: and Bonneau, O., “Performance based specifications of self-consolidating concre te used in structural applications,” ACI Materials Journal, V.103, No.2, March-April 2006, pp 121-129. [30]. Shindoh, T. and Matsuoka, Y., “D evelopment of combination type self- compacting concrete and evaluation test methods”, Journal of Advanced Concrete Technology, Vol.1, No.1, 26-36, April 2003, Japan Concrete Institute. [31]. Rizwan, S. A., and Bier, T. A., “Inc lusion of Mineral Admixtures in Cement Pastes for High Performance Concrete”, 2 nd International Conference on ”Concrete and Development”, CD7-004, April 30-May 2, 2005. Tehran. Iran. pp 1-12. [32]. Rizwan, S. A., and Bier, T. A., “Role of Mineral Admixtures in High Performance Cementitious Systems”, International Conference on “Concrete and Reinforced concrete”, 2nd All Russian International Conference on “Concrete and reinforced Concrete-Development trends”, Vol. 3, “Concrete Technology”, 5-9 September 2005, Mosco, Russia. pp 727-732. [33]. Rizwan, S. A., and Bier, T. A., “Ear ly Volume Changes of High-Performance Self-Compacting Cementitious Systems Containing Pozzolanic Powders”, Paper accepted for International RILEM Conference on Volume Changes of Hardening Concrete: Testing and Mi tigation” Lyngby, Denmark, 20-23 August 2006 [34]. Khayat, K. H; Assad, J: and Daczko , J., “Comparison of field oriented Test methods to Assess Dynamic stability of self-consolidating concrete”, ACI materials Journal, V. 101, No. 2, March-April 2004, pp 168-176. [35]. Struble, L. J., and Jiang, Q., “Effects of air Entrainment on Rheology”, ACI Materials Journal, V. 101, No. 6, November-December 2004, pp 448-456.
Filename:
Paper670.pdf
File Type:
pdf
File Size:
865 KB
Downloads:
1
