Paper No. 679 COMPARATIVE STUDY OF NYLON AND PVC FLUIDIZED BED COATING ON MILD STEEL R. Ahmad, S. Aziz, J. Iqbal 438 Ahmad, Aziz, Iqbal Pakistan Engineering Congress, 70th Annual Session Proceedings 439 COMPARATIVE STUDY OF NYLON AND PVC FLUIDIZED BED COATING ON MILD STEEL R. Ahmad1, S. Aziz1, J. Iqbal2 ABSTRACT The present study is the result of an experimental investigation of the fluidized bed coating on mild steel specimens using Nylon-11and PVC powders. The effects of dipping time and preheat temperature on coating thickness were investigated. A preheat temperature of 265 oC to 270oC for PVC and 350oC to 360oC for Nylon-11 is necessary to achieve an acceptable surface. The optimum thickness of 930 microns for nylon and 1407 microns fo r PVC was obtained on mild steel. To minimize errors in achieving the desired coating thickness, dipping time shorter than 5 sec is not recommended. Fluidized bed coating process does not require solvents and thus provides an environm entally friendly alternative to other techniques such as dipping, brushing, spraying etc. It also offers the advantage of efficient utilization of materials (nearly 100%), the ability to coat irregular shapes, high coating rates, simple and inexpensive equipment requirements, process automation, smooth and continuous coat ing applications. Graphs of coating thickness versus dipping time presented in this study enable the optimal choice of preheat temperature and dipping time to achieve the acceptable surface finish. Keywords: Coating, Fluidized bed Coating, Ny lon and Poly vinyl chloride (PVC) coating on mild steel. 1 College of Engineering & Emerging Technologies, University of the Punjab, Quaid-e-Azam Campus (New Campus), Lahore, PAKISTAN 2 Department of Metallurgical & Materials Engine ering, University of Engineering & Technology, Lahore, Pakistan 440 Ahmad, Aziz, Iqbal INTRODUCTION Coatings are substances applied to th e surface of a substrate to modify the functional properties of th e substrate. Such surface mo dification dates from very early in the technical development of man. Coatings are used most frequently for protection of metal surface for corrosion protection, coating of wood to prevent decay and wrapping of food products with coated film to prevent spoilage [1]. Coating processes fall in the area of polymer fabrication technologies along with molding, extrusion, casting, forming and calendaring. In parts that must be constructed of metal for structural reasons, a plastic coating may be applied for decorative and /or functional purposes such as electrical insulation, corrosion protection and abrasion resistance. Thin film powder coating, also referred to as a “dry painting” process, eliminates volatile organic compounds (VOCs), hazardous air pollutants, solvents and produces superior surface finish. There are four basic powder coating application processes, dip coating, electrostatic spraying, fluidized bed, and flame spray. For all application methods, surface preparation (i.e., cleaning and sometimes application of a conversion coating) is required to develop good coating adhesion to the work piece surface. A Fluidized bed is an amazing thing to see. Plastic powder is fluidized by gently blowing air into the bottom of the tank and through a diffusion plate and finally, through the powder. Before the powder is fluidized, it’s about as penetrable as fine beach sand. Once the air goes on, the bed rises about 30%, and looks like its boiling at the surface. If hand is put into the bed, it goes in with no resistance at all, (and the bubbles tickle). The part to be coated is preheated in an oven, and then dipped into the fluidized bed. As powder particles come in contact with the hot parts, they melt on creating the plastic coating. The plastic coating builds up quickly and uniformly. After the part is withdrawn, there may be enough heat left to completely fuse the coating and even melt the surface smooth. If there is enough residual heat, just cool, inspect and pack. Otherwise the part is returned to the oven for a very short time. The coating may be reheated to achieve a smoother finish. For a given object, the thickness of the coating is dependent on two process variables; preheat temperature of the object, and the amount of time for which it is immersed in the powder [2]. Fluidized bed plastic coatings usually are in the thickness range of 300-2000 microns. However, K.C Leon g, G.Q.Lu, B.Rudolph [3] reported that coating thickness less than 400 micron is difficult to achieve with Nylon-11. K.C Leong and G.Q.Lu also reported increase in coatin g thickness with increase of preheat temperature and dip time [4]. Thicker coatings require using multiple dips or plastisol coating. Fluidized bed coatings have the tremendous advantage of being remarkably uniform in thickness. These coatings eliminate the need for expensive and often toxic solvents, the control equipment, employee exposure, and the disposal Pakistan Engineering Congress, 70th Annual Session Proceedings 441 requirements and liabilities associated with liquid coating (wet solvent) use. Because the powder is dry when fluidized, and overspray can be readily retrieved and recycled, regardless of the complexit y of the system, resulting in shorter cleanup times. In all cases, the dry powder is separated from air stream by various vacuum and filtering methods and returned to a feed hopper for reuse. Powder efficiency (powder particles reaching the intended surface) approaches 100 percent. Other advantages over conventional spray painting include greater durability; improved corrosion resistance; electropla ting; electrical insulation; ease of cleanliness; availability in any colour; and elimination of drips, runs and bubbles. Fluidized bed technique has been used to coat discrete objects and continuous webs such as wires, wire fencing and rolls of metal foil. Successful users now consider it as integrated finish system incorporated into production for the purpose of providing corrosion protection, abrasion resistance, electrical insulation and for decorative purposes. Typical applications include the coatings of rotors and stators in electric motors and generators; pipes, fittings and valves in fluid conveying systems, components of electrical appl iances such as dishwashers, washing machines, refrigerators and for automotive components [3]. Parts can be coated with polyvinylchl oride, nylon, polyethylene and epoxy. Fluidized bed plastic coatings are usually applied to metals, ceramics and glass. In Fluidization, a gas or liquid is passed through a bed of solid particles, which is supported, on a perforated or porous plate. In the case of fluidized bed coating, air is passed through a bed of polymer particles. When the pressure drop of the flowing air through the bed equals or exceeds the weight of the bed, the powder particles become suspended and the bed exhibits liquid-like behavior. As shown in the figure 1, at gas flow rates less than the fluidization velocity, the bed is fixed bed and there is no movement of particles. At flow rates above minimum fluidization the bed expands and bubbles appear. The air velocity corresponding to a pressure drop that just equals the weight of the bed is referred to as the minimum fluidization velocity. At this flow rate all of the be d particles are completely suspended by the air stream. For a given system, minimum fluidization velocity can be determined from a pressure drop vs. air velocity diagram [4]. As airflow is increased above the minimum fluidization velocity, the bed may exhibit behaviors ranging from smooth fluidization to dilute fluidization in which powder can be transported by the air stream. Smooth fluidization is desirable for optimal performance in the powder coating process. The liquid-like nature of the fluidized powder bed allows a metal object to easily be dipped into it. Polymer Powders In present study two types of polymer powders Nylon-11 and polyvinyl chloride were used for coating mild steel. Nylon-11 has been used almost exclusively because it has low melt viscosities than Nylon-6,6. Nylon coating powders are available for electrostatic spray and fluidi zed-bed application. Nylon coatings are very tough, resistant to scratching and marring, have a pleasing appearance, and are suitable for food contact applications when properly formulated. These coatings 442 Ahmad, Aziz, Iqbal are used for chair b ases, hospital furniture, office equipment, knobs, ha ndles, and other hardware.. Nylon coatings have good solvent and chemical resistan ce and are used fo r d ishwasher basket s, food trays, hot wate r heaters, plating and chemical etching racks, and large diameter water pipes in power-generating stations. Dishwasher baskets are coated with fluidized bed PVC powder. Other applications are wa shing machine retainer rings and various types o f wire me sh and chain -link fencing. PVC coatings have a cost /performance balan ce that is difficult to match with any of the ot her thermoplastic materials. Properl y formulated PVC powders have good outdoor weathering resistance and are used in many applications where good corrosion re sistance is required. These coatings are also resistant to attack by most dilute chemicals except solve nts. In addition PVC coatings achieve exc ellent edge coverage by fluidiz ed bed coating techni que, which cannot be achieved by other techniques. EXPERIMENTAL Eq uipment Design Mechanical Hanging Wire Porous plate Figure. 1: Setup for Fluidized bed coating. The fluidized bed was fabricated from clear Plastic (acrylic) tube wit h a diameter of 3.3” and a height of 60”. A distribution chamber is attached at the lower end of the tube to produce uniform fluidi zation throughout the bed. Dry air enters the bed through the distribution cham ber through a regulating valve. The distributor plate is a polyethylene porous sheet manufactured specifically for heat- treating fluidized beds. The drop mechanism for th e metal samples was fabricated by bending stainless steel tubing into a U-shape and running a thin metal cable through the center of the tube. An attachme nt device was placed at one end to hook Pakistan Engineering Congress, 70th Annual Session Proceedings 443 a wire loop to it and the other end had an adjustable stop. Figure-1 illustrates the complete set up of apparatus. Specimens Mild steel specimens were cut from a sheet having dimensions 2.5” x 1.5” x 0.25”. A small hole having diameter of 0.15” was grooved in the samples at the centre of the top for hanging the samples with metallic wire in the fluidized bed. Surface Preparation of Specimens Surface of specimens were prepared to remove any grease, dirt and oxide. This was done by first of all dipping th e specimens in alkaline cleaning solution having a composition 5%Na 2CO3, 5%NaHCO3, 2%Trisodium Phosphate, 0.5% Fatty Acid Ester to remove any organic soils present on the surface followed by rinsing in water. Then the specimens were pickled in 5%H2SO4 followed by neutralization and rinsing to remove any oxide present on th e surface. Pickled specimens were then immersed in iron phosphate solution to ac hieve phosphate coating over the surface. This surface preparation technique will serve to achieve better adhesion and uniformity in the coating with superior corrosion protection. Sieve Analysis of the Powders The powders were sieved using standard sieves (Tyler, USA). The mean particle size of Nylon-11and PVC calculated from the sieved mass fractions was 106 micron and 63 micron respectively. Procedure for the Coating Powders were dried prior to coating in the oven at temperature of 105 oC to drive off any moisture present. The powder was placed in the fluidized bed and the air was blown from the bottom at high pressure to mix the powder thoroughly for a few minutes. Then the airflow rate was adju sted to achieve a fluidization condition in the bed. Coating experiments were performed at a fluidization velocity of 0.02 m/s as shown in figure. 2, which is higher than the minimum fluidization velocity as it is obvious from graph figure. 3 for ac hieving boiling liquid like situation in the fluidized bed powder to enable the metal specimens easily dipped in the fluidized bed. Specimens were preheated at various temperatures and were immersed in the fluidized bed for different time interv als. Then the specimens were withdrawn from the bed and allowed to cool in air followed by water quenching. This would ensure excellent surface finish of the coating with minimum defects. Both nylon-11 and PVC coating were applied at different preheated temperatures and time. Coated specimens were cut transverse to their cross-section and coating thickness was measured by using ocular micrometer. 444 Ahmad, Aziz, Iqbal Low Air Flow Rate Fixed bed 0.008m/s – 0.013m/s Moderate Air Flow Rate Minimum fluidization 0 013 / High Air Flow Rate Bubbling Fluidization 0.019 – 0.020m/s Figure. 2: Fluidization Regimes. Determination of Minimum Fluidization 0.0 0.5 1.0 1.5 2.0 2.5 3.0 3.5 0.00E+00 1.00E-04 2.00E-04 3.00E-04 4.00E-04 5.00E-04 Flowrate (m3/s) Bed Pressure Drop (in H2O) Figure 3: Determination of Minimum Fluidization. RESULTS AND DISCUSSION Preheating temperature about 100 oC above the fusion point of powders, which is 3 60oC for Nylon-11 an d 270oC for PVC were selected, at this temperature Pakistan Engineering Congress, 70th Annual Session Proceedings 445 powder particles fuse together to form a co ntinuous film. In all cases it is observed that coating is formed at the rapid rate when the specimen is dipped in the fluidized bed. Generally graph shows that coating thickness increases with time. y = -5.9819×2 + 186.28x – 480.55 200 300 400 500 600 700 800 900 1000 1100 1200 0 5 10 15 20 25 Dip Time (sec) Coating Thickness (microns) At temp 360 deg celcius Figure. 4: Coating thickness in microns Vs Dip time (sec) for Nylon coating at 300oC. It can be seen from figure. 4 that th ickness of Nylon-11 coating on mild steel increases linearly with dipping time, re aching to maximum thickness of 930 microns at 360oC in 13 seconds, however there is no any significant incre ase in the coating thickness with increase of dipping time as shown in Table 1. However an acceptable coating of minimum thickness of 300 microns for Nylon-11 is achieved in a dip time of 5 sec. It was also observed that some particles of powder get adhere to the surface without fusing because there is no enough heat available f or melting due to insulation caused by Nylon-11 coating. Table 1: Effect of dipping time on coating thickness at 360oC for Nylon coating. Dip time(s) 5 7 8 9 10 12 13 15 16 19 20 Coating thickness (micron) 300 425 625 790 900 895 930 900 895 905 900 446 Ahmad, Aziz, Iqbal At temp 270 deg celcius y = -0.4014×2 + 34.642x + 656.64 600 700 800 900 1000 1100 1200 1300 1400 1500 0 10 203 0 405 06 0 Dip Time (sec) Coating Thickness (microns) Figure 5: Coating thickness in microns Vs Dip time (sec) for PVC coating at 270oC. It may be observed from fig-5 that coating thickness of PVC also increases with increase of dipping time, reaching to a maximum thickness of 1407 microns at 270oC in 35 sec, afte r that there is no any significant increase in coating thickness as also shown in Table 2. It was also observed that some of the powder remained attach over the prev ious coati ng layer can be fuse d by post coating treatment by placing the sample in the oven at a temperature of 270±10 oC until uniform coating is achieved. Table 2: Effect of dipping time on coating thickness at 270oC for PVC coating. Dip time(s) 5 10 20 25 30 35 40 45 50 Coating thickness (micron) 848 945 1128 1288 1360 1407 1400 1388 1380 Pakistan Engineering Congress, 70th Annual Session Proceedings 447 CONCLUSIONS 1. Maximum thickness i.e. 930 microns of Nylon-11 coating on mild steel was achieved at a preheat temperature of 360oC with a dip time of 13 second. 2. The minimum coating thickness of 300 microns of Nylon-11 was obtained in 5-second dip time. 3. Uniform PVC coatings of thickness 1407 microns can be achieved at preheat temperature of mild steel 270 oC with dip time of 35 second. It was further monitored that with increase of dip time there was no any significant increase in coating thickness of PVC beca use of very less heat is available for melting the resin particles. 4. Mild steel was found a better material for fluidized bed coating process. REFERENCES 1 . Hesketh, R. P., C. S. Slater, S. Farrell, and M. Carney, “Fluidized Bed Polymer Coating Experiment”, Chemical Engineering Education Rowan University, Vol. 36(2), 2002, p138. 2. Pettigrew C. K. “Effects of dipping, post heating and complex geometrical variables”, Fluidized bed coating – Part 2, Mod. Plastics vol. 44, 1966: pp150- 156. 3. K.C Leong, G.Q.Lu, V.Rudolph. “A co mparative study of the fluidized-bed coating of cylindrical metal surfaces with various thermoplastic polymer powders”, Journal of Materials processing Technology, Elsevier, Vol. 89-90, 1999, pp.354-360 4. Leong K.C, Lu G.Q. “Fluidized bed coat ing of copper Cylinders”, Journal of Materials processing Technology, Elsevier. Vol. 48, 1995 pp. 525-531 5. Rodriguez, F: “Principles of Polymer Systems”, Hemisphere Publishing Corporation, Washington. 1982 6. Kunii, D. and Levenspiel, O.: “Fluidization Engineering”, Butterworth- heinemann, Boston. 1991 7. Narikis, M. and Rosenzweig, N.: Polymer Powder Tecnology, Wiley, Chichester. 1995 8. Gaynor, J., Chemical Engineering Progress, Vol. 7, 1960 p.75. 9. Charles A. Harper. Handbook of Plastics, Elastomers, and Composites, 3rd ed. McGraw-Hill, New York, 1996, 6.38. 448 Ahmad, Aziz, Iqbal
Filename:
Paper679.pdf
File Type:
pdf
File Size:
79 KB
Downloads:
1