Paper No. 676 SYNTHESIS AND APPLICATIONS OF TiO2 NANOPARTICLES Dr. A. Ahmad, Gul Hameed Awan, Salman Aziz 404 Ahmad, Awan, Aziz Pakistan Engineering Congress, 70th Annual Session Proceedings 405 SYNTHESIS AND APPLICATIONS OF TiO2 NANOPARTICLES Dr. A. Ahmad1, Gul Hameed Awan1, Salman Aziz1 ABSTRACT Nanocrystalline semiconductor metal oxides have achieved a great importance in our industrial world today. They may be defined as metal oxides with crystal size between 1 and 100 nm. TiO 2 nanosize particles have attracted significant interest of materials scientis ts and physicists due to their special properties and have attained a great importance in several technological applications such as photocatalysis, sensors, solar cells and memory devices. TiO 2 nanoparticles can be produced by a variety of techniques ranging from simple chemical to mechanical to vacuum methods, including many variants of physical and chemical vapor deposition techniques. In the present research work we report the synthesis of TiO2 nanoparticles by Sol-Gel technique. The characterization of particles was carried out by XRD, TEM and XPS techniques. The importance and applications of these nanoparticles are discussed in detail. 1 Department of Metallurgical and Materials Engineering University of Engineering and Technology, Lahore. 406 Ahmad, Awan, Aziz INTRODUCTION Nanocrystalline semiconductor TiO 2 particles are of interest due to their unique properties and several potential technological applications such as photocatalysis, sensors, solar cells and memory devices (1-4). TiO 2 exists in three polymorphic phases: rutile (t etragonal density = 4.25 g/cm 3), anatase (tetragonal, 3.894 g/cm3) and brookite(orthorhombic, 4.12 g/cm 3). Both anatase and rutile have tetragonal crystal structures but belong to different space groups. Anatase has the space group I4 1/amd (4) with four formula units in one unit cell and rutile has the space group P4 2/mnm (5) with two TiO 2 formula units in one unit cell (5,6). The low-density solid phases are less stable and undergo transition rutile in the solid state. The transformation is accelerated by heat treatment and occurs at temperatures between 450 and 1200oC (7). This transformation is dependent on several parameters such as initial particle size, initial phase, dopant concentration, reaction atmosphere and annealing temperature, etc. (8-11). Crystal Structure of TiO2 Among the three above mentioned crystal structures of TiO 2, anatase owing to its higher photocatalytic activity is co mmonly used for photocatalysis (12). This higher photocatalytic activity is related to its lattice structure. Each Ti atom is coordinated to six oxygen atoms in anatase tetragonal unit cell. Yong et.el. (12) have reported a significant degree of bu ckling associated with O-Ti-O bonds in anatase compared to rutile TiO 2. Crystal symmetry is reduced due to this buckling and in turn it results a larger unit cell dimensions in the (001) direction. The kinetics of phase transformations in TiO 2 is extensively reviewed by Zhang & Banfield et al (6, 8, 9). Fig.1 shows the unit cell structures of the anatase and rutile crystals. The titanium and oxygen atoms are more tightly packed in the rutile crystal. Both structures can be described in terms of chains of TiO 2 octahedra. Each Ti +4 ion is surrounded by an octahedron of six O -2 ions. The octahedron in rutile is not regular, showing a slight or thorhombic distortion. The octahedron in anatase is significantly distorted so that its symmetry is lower than orthorhombic. The Ti-Ti distance in anatase is greate r whereas the Ti-O distances are shorter than in rutile. In the rutile structures each octahedron is in contact with 10 neighbor octahedrons (two sharing edge oxygen pairs and eight sharing corner oxygen atoms) while in the anatase structure each octahedron is in contact with eight neighbors (four sharing an edge and four sharing a corner). These differences in lattice structures cause different mass densities and electronic band structures between the two forms of TiO 2 as indicated in Fig.1. Anatase can be conceived as an arrangement of parallel octahedral, while in case of rutile some octahedral are rotated by 90o. There is a symmetry change from I4 1/amd to P42/mnm space group in terms of reconstructive polymorphism during conversion from anatase to rutile. As a consequence, the ionic mobility that o ccurs during phase transition results in increased densification and coarsening of the TiO2 nanoparticles (6, 8, 9). Pakistan Engineering Congress, 70th Annual Session Proceedings 407 a = 3.784 Ao c = 9.515 Ao a = 4.593Ao c = 2.959 Ao (a) (b) Fig. 1 Structure of anatase and Rutile TiO2 (a) anatase (b) rutile TiO 2 is stable in aqueous media and is to lerant of both acidic and alka line solutions. It is inexp ensive, recyclable, reusable and relatively simple to produce. It can also be synthesized in nanostructur e form s more read ily than many other catalysts. Furthermore, its bandgap is ap propriate to initiate a variety of organic reactions. Semiconductor photocatalysis uses su nlight to activate nanopar ticles catalysts to break down these chemicals. Photocatalysis works on the principle that light falling on a semiconductor with an appropriate bandgap, or energ y difference between the conduction and the valanc e bands will create positive (holes) and negative (electrons) charge carriers, whi ch can in turn be used to initiate reduction (electrons) and oxi dation (holes) reactions at the catalyst surface. Several competing effects in herently limit catalyst efficiency. The positively charged holes and negatively charged electro ns tend, b y nature, to recombi ne to yield a neutral state, through reemission of a photon (light ) or a phonon (heat). This can occur via volumetric and surface reco mbination. Nanostructured (~20-30nm) particles provide th e optimal balance between these effects and are thus best suited to photocatalysis. An additional advantage ob tained in nanoparticles in the few ten s of nm size regime is that the large surface /volume ratio makes possible the timely utilization of photogenerated carriers in interfacial processes (4,5). TiO 2 nanoparticles can be synthesized us ing various methods such as su lfate process (13), chloride proce ss (13), i mpregnation (14), coprecipita tion (15), hydrothermal method (16-18), direct oxidation of TiCl4 (19), metal organic chemical vapor deposition me thod, etc.(1, 20). S ol-gel method (21-23) is one of the most convenient ways to synthesiz e various metal ox ides due to low co st, ea se o f fabrication and low processing temperatures. It is widely used to prepare TiO2 for films, particles or monoliths. In general, the sol gel process involves the transition of a syste m from a liquid “sol” (mostly colloidal) into a solid “gel” phase. The homogeneity of the gels depen ds on the so lubility of reagents in the solvent, the sequence of addition of reactants, the temperature and th e pH. Th e precurso rs normally used for the synthesis and doping of nanoparticles are organic alkoxides, 408 Ahmad, Awan, Aziz acetates or acetylacetonates as well as inorganic salts such as chlorides. Among the classes of solvents, alcohols are largely used but other solvents such as benzene may also be used for some alkoxides. Experimental The titania nanoparticles were synthesized by drop wise additi on of titanium tetrachloride: TiCl4 (Fluka 98%) in ethanol (Pharmco 200 proof). The reaction was performed at room temperature while stirring under a fume hood due to the large amount of Cl2 and HCl gases evolved in this reactio n. The resulting yellow solution was allowed to rest and cool back to room temperature as the gas evolution ceased. The suspensions obtained were dried in an oven for several hours at 80 oC until amorphous and drie d TiO2 particles were obtained. The obtained powde r samples were calcined for one hour in a box furnace at temperature ranging from 300 to 85 0 oC in an ambient atmosph ere. To study the time dependence of phase transformation and particle g rowth rate, samples were also calcined by varyin g calcinations time for 0.5 to 2 hours. XR D patterns were reco rded on as prepared and calcined sample s using a Rigaku D-Max B diffracto meter equipped with a graphite crystal monochromator, operating with a Cu anode and a sealed X-ray tube. The 2 Θ scans were recorded at several resolu tions using Cu K α radiation of wavelength 1.54 Å in the range 20-80 o with 0.05o step size. The recorded patterns were analyzed using Jade ® software to determi ne peak position, width an d intensity. Full-width at half- maxima ( FWHM) data was analyzed by Scherer’s formula (equation N o.1) to determine averag e particle size. Scherer’s equation i s given by θβ λ Cost 9.0= (eq.1) where λ is the X-ray wavelength, β is the peak width and theta is the Bragg’s angle. Since peak width u sed in the Scherer’s formula also include s the line broadening due to strain in the particles, measurements of pa rticle size and distri bution were also carried out by TEM. Both bright fi eld and dark field micrographs were taken with a JEOL JEM-2000FX operating at 200 kV. Samples for TE M were prepared by dropping a dilut e suspension of the sample powders onto a 300-mesh Lacy carbon grid. Dilute suspension was prepa red by son icating the particles i n acetone for 5 to 10 minutes. The lattice constant s of calci ned sa mples was al so measured. For this analysis only samples containing the anatase phase were used, to avoid the effect of rutile crystals segregated out of anatase system. Samples were annealed at 500 oC for 1 hour before analysis for XRD. The peak positions (2θ) of the anatase (101) and (200) reflections were used to calculate the lattice parameters using the followin g formula (equation 2) 2/1)///( 1 clakah d ++ = (eq.2) Pakistan Engineering Congress, 70th Annual Session Proceedings 409 The value of d, for an XRD peak can be determined from the 2 θ angle by Bragg’s Law (Eq.3) d = θ λ sin2 (eq.3) where λ is the X-ray wavelength and θ is in radians. The mass fraction of rutile (X r) in the samples calcined at vari ous temperatures was calculated based on the relationship between the integrated intensities of anatase (101) and rutile (110) peaks by th e following formula developed by Spurr and Myers Xr = )/1( 1 ra IKI+ (eq. 4) where I a and I r are the integrated peak intensities of anatase and rutile peaks respectively. The constant K was determined previously by A. Burns et al (16) and Barakat et al (20 ) via an XRD anal ysis of stan dard mixture of TiO 2 powder (Degussa P-25) of known proportions of an atase and rutile (80:20) and is equal to 0.79. The activation energy, Ea for the anatase to rutile phase transformation were calculated from the slope of the plot of the corrected rutile weight fractions, Xr as a function of the reciprocal of annealin g temperature from XRD spectra. The relationship is given as below: TR EX a r 1ln −= (eq. 5) 1000)/1( )ln( R T XrEa ∂ ∂−= (eq. 6) where Ea is the anatase to rutile transformation activation energy, T is temperature in Kelvin, R is the universal ga s constant (8.314 J/mol K) and X r is the corrected weight fraction of rutile as defined earlier. Results and Discussion: Fig.1 shows the X-ray diffraction pattern for as-prepared TiO 2 synthesized via so-gel route. As prepared nanosize particles showed a morphous structure. Fig.2 shows the XRD patterns of TiO 2 samples annealed at various temperatures. Annealing resulted in diffraction peaks related only to the anatase and rutile polymorphs of TiO 2. From 300 oC to 650 oC only peak s related to anatase structure were evident. Above 650 oC rutile peaks sta rted to appear and a 20 25 30 35 40 45 50 55 60 65 70 75 80 400 410 420 430 440 450 460 470 480 Fig 1- X-ray diffraction pattern as synthesized TiO2 nano particles. Intensity (Arbitratory units) Bragg’s Angle (2Θ) amorphus 410 Ahmad, Awan, Aziz mixture of both the anatase and ruti le phases of TiO existed up to 800 2 oC. At 850 oC, the XRD pattern showed a complete transformation from anatase to rutile. From the XRD data of Fig. 2, it is evident that the crystallite size increases with increasing calcinations temperature and that the diffraction peaks become intense a nd their FWHM gradually became narrow suggesting an increase in particles size and increa se in the amount of the pertinent phase. The anatase (101) peak was used to determine the grain size by Scherer’s formula. The results of the grain size analysis is shown in Fig. 3. 20 25 30 35 40 45 50 55 60 65 70 75 80 0 1000 2000 3000 4000 5000 6000 7000 8000 9000 10000 A(215)A(220)A(204)A(211)A(105)A(200) A(116)A(004)A(101) R(112)R(002) R(310) R(301)R(220)R(211)R(210)R(111)R(101)R(110) 900 o C 850 o C 800 o C 750 o C 700 o C 650 o C 600 o C 500 o C 450 o C 400 o C 350 o C 300 o C Amorphous Fig 2- X-ray diffraction patterns of TiO2 annealed at various temperatures. Intensity (Arbitratory units) Bragg’s Angle (2Θ) 250 300 350 400 450 500 550 600 650 700 10 20 30 40 50 60 70 Fig 3- Variation of particles size as a function of calcination temperature. Particle size of anatase (nm) Temperature oC size The particle size of TiO2 annealed at various temperatures was also analyzed by TEM. Figures 4 show the TE M bright field image, of Ti O2 at 500 oC for 1 ho ur. The particles size measured by TEM we re generally in agreement with those determined by XRD though some agglomeration is present due to high surface energy of the particles. The TiO2 anatase unit cell i s tetragonal with latti ce parameters “a” and “c” corresponding to 3.78 and 9.52 Å, respectively. Rutile is also tetragonal with “a” and “c” parameters as 4.59 and 2.96 Å, respectively. The lattice constants a and c of anatase structure were determin ed by XRD. This analysis was performed on samples annealed at 500 oC for 1 hour, i.e., well below the anatase to rutile transformation temperature, in order to avoid the effects of rutile crystal precipitating out of the anatase lattice. The peak values of the anatase (101) and (200) reflections were used to calculate the lattice parameters. The lattice parameter a and c were in good agreement with the literature. Figure 4- EM bright field image of TiO2 annealed calcined at 500oC for one hour. Pakistan Engineering Congress, 70th Annual Session Proceedings 411 Fig.5 shows the effect of calcination temperature on the anatase to rutile phase transformation for undoped TiO 2 samples. Mass fraction of rutile phase was calculated according to the equ ation 3, b ased on the integrated intensity ratio(Ir/Ia) of rutile and anatase XRD peaks. The peaks chosen for the cal culation of this ratio were (101 ) and (110) peaks as the anatas e and ruti le peaks, respectively. Tables 1 summarize the XRD results showing the p ercentage of phases observed for undoped samples. 650 700 750 800 850 0.0 0.2 0.4 0.6 0.8 1.0 Fig 5- Effect of calcination temperature on the anatase to rutile phase transformation for TiO2 nano particles. mass fraction Xr Temperature oC Xrundoped Temperature Time %Rutile %Anatase 40 oC 48hrs Amorphous 300 oC 1hr 0 100 350 oC 1hr 0 100 400 oC 1hr 0 100 450 oC 1hr 0 100 500 oC 1hr 0 100 600 oC 1hr 0 100 650 oC 1hr 0 100 700 oC 1hr 24 76 750 oC 1hr 78.7 21.3 800 oC 1hr 96.9 3.1 850 oC 1hr 100 0 900 oC 1hr 100 0 As expected, the percentage of rutile phase increased with the increase in calcination temperatures. Table-I: % age of Phases observed. CONCLUSIONS • As prepared TiO2 particles are amorphous in nature. • Amorphous to anatase transformation started at temperature above 250oC. • Anatase was stable upto temperature 650oC. • The anatase-to-rutile transformation started at temperature above 650oC. • Mass fraction of rutile was increas ed with the rise in calcination temperature. • Particle size of anat aze was increased as the calcination temperature was increased. REFERENCES 1. W.Li, S.Ismat Shah, C.P Huang, O.Jung and C. Ni, Mater. Sci.Eng. B 96, 247 (2002) 412 Ahmad, Awan, Aziz 2. J.T.Remillard, J.R.McBride, K.E.Nietering, A.R.Drews and X.Zhang, J.Phys.Chem.B104, 4440 (2000) 3. E.Traversa, J.Am.Ceram.Soc.78, 2625 (1995) 4. A.I.Kingon, J.P.Maris and S.K.Steiffer, Nature (London) 406, 1032 (2000) 5. W.Li, C.Ni, H.Lin, C.P.Huang and S.Isma t Shah, Journal of Applied Physics, Volume 96, No.11, 6663 (2004) 6. H.Zhang.and J.F.Banfield, Am.Mineral.84, 528 (1999) 7. A. Tsevis, N. Spanos, P. G. Koutsoukos, Ab J. Van der Linde and J. Lyklema, J. Chem.Soc, Faraday Trans; 94(2), 295 (1998) 8. H. Z. Zhang and J.F.Banf ield, J.Mater.Chem. 8, 2073 (1998) 9. H.Z.Zhang and J.F.Banfie ld, J.Phys.Chem.B 104, 3481(2000) 10. M.R.Ranade, A.Navrotsky, H.Z.Zha ng, J.F.Banfield, S.H.Elder, A.Zaban, P.H.Borse, S.K.Kulkarni, G.S.Doran and H.J.Whitfield, PNAS99, 6476 (2.11.02) 11. J.Arbiol, J.Cerda, G.Dezanneau, A.Cirera, F.Peiro, A.Cornet and J.R.Mornate, J.Apply.Phy.92, 853 (2002) 12. Yong Liang, Shupan Gan, Scott A. Chambers and Eric I.Altman, Physical Review B, Vol. 63, 235402-1 (2001) 13. M. Howe.Grant (Ed), Kirk-Othmer Encyclopedia of Chemical Technology, vol.24, John Wiley & Sons, Inc, p.225, 1997 14. M.I.Litter, J.A.Navio, J.Photoc hem.Photobiol.A.Chem.84 183, (1994) 15. L.Palmisano, V.Augugliaro, A.Scla fani. M.Schiavello.J.Phys.Chem.92, 6710 (1988) 16. Y.Wang.H.Cheng.Y.Hao.J.Ma. W. Li . S.Cai, J. Mater.Sci 34, 3721(1999) 17. H. Cheng. J.Ma, Z.Zhao, L.Qi, Chem.Mater. 7, 663 (1995) 18. Y.Wang, Y.Hao, H.Cheng, J.Ma, B. Xu, W. Li, S. Cai, J. Mater. Sci. 34, 2773 (1999) 19. M.K.Akhtar, Y.Xiong, S.E. Pratsinis, AIChE J.37, 1561(1991) 20. Z.Ding, X.Hu.G.Q.Lu, P.L.Yue, P.F.Greenfield, Langmuir 166216 (2000) 21. C.C.Wang, Z.Zhang, J.Y.Ying, Na noStructured Mater. 9, 583 (1997) 22. A.Burns, W.Li, C. Bake r, S.I.Shah, Mater. Res. Soc. Symp. Proc.V.5.2.703 (2002) 23. Andrew Burns, G.Hayes, W.Li, J.Hi rvonen, J.Derek Demaree, S.Ismat Shah, Materials Science and Engineering, BXXX MSB 9793 1-6 (2004) 24. F.M.F.de Groot and J.C.Fuggle, Physics Review B vol 41 No.2, 928(1990)
Filename:
Paper676.pdf
File Type:
pdf
File Size:
257 KB
Downloads:
2